For Heat-resisting Steel
|
|
Brand Name
|
Type of covering
|
Equivalent Specification
|
Welding Position
|
Type of Current
|
Chemical Composition of Wire(%) |
Mechanical Properties of
Deposited Metal
|
Applications |
|
C
|
Mn
|
Si
|
S
|
P
|
Cr
|
Mo
|
V
|
|
Y.P(MPa)
|
T.S. (MPa)
|
EL.(%) L=5d
|
Typical
I.V.(J)
|
|
CHH107 |
Low hydrogen sodium
|
AWS E7015-A1
GB E5015-A1
|
F, V,
OH, H
|
DC+
|
<=0.12
0.08
|
<=0.90
0.70
|
<=0.60
0.40
|
<=0.035
0.020
|
<=0.035
0.020
|
-
|
0.40-0.65
0.50
|
- |
- |
>=390
440
|
>=490
550
|
>=22
26
|
20oC
120
|
Welding of boiler
pipeline, working temperature of which is below 510oC and also
suitable for that of normal low alloy high strength steels.
|
|
CHH108 |
Low hydrogen
potassium
|
AWS E7015-A1
GB E5015-A1
|
F, V,
OH, H
|
AC or DC+
|
<=0.12
|
<=0.90
|
<=0.80
|
<=0.035
|
<=0.035
|
-
|
0.40-0.65
|
- |
- |
>=390
|
>=490
|
>=22
|
20oC
>=27
|
Welding of boiler
pipeline, working temperature of which is below 510oC and also
suitable for that of normal low alloy high strength steels.
|
|
CHH202 |
Lime titania
|
GB E5503-B1
|
F, V,
OH, H
|
AC or DC+
|
0.05-0.12
0.07
|
<=0.90
0.70
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.40-0.65
0.50
|
0.40-0.65
0.50
|
- |
- |
>=440
480
|
>=540
590
|
>=16
23
|
-
|
Welding of boiler
pipeline, working temperature of which is below 510oC and also
suitable for that of normal low alloy high strength steels.
|
|
CHH207 |
Low hydrogen sodium
|
AWS E8015-B1
GB E5515-B1
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
<=0.90
0.70
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.40-0.65
0.50
|
0.40-0.65
0.50
|
- |
- |
>=440
480
|
>=540
590
|
>=17
23
|
20oC
>=
27
|
Welding of low alloy
CrMo pearl tic steels, such as 2CrMo etc, working temperature of which
is below 510oC .
|
|
CHH307 |
Low hydrogen sodium
|
AWS E8015-B2
GB E5515-B2
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
<=0.90
0.70
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.80-1.50
1.20
|
0.40-0.65
0.50
|
-
|
-
|
>=440
500
|
>=540
600
|
>=17
23
|
20oC
>=
27
|
Welding of low alloy
CrMo pearl tic steels, such as 2CrMo etc, working temperature of which
is below 510oC .
|
CHH308 |
Iron power Low hydrogen
potassium
|
AWS E8018-B2
JIS DT2318
|
F, V,
OH, H
|
AC or DC+
|
0.05-0.12
0.07
|
<=0.90
0.70
|
<=0.80
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.80-1.50
1.20
|
0.40-0.65
0.50
|
- |
- |
>=440
500
|
>=540
590
|
>=17
23
|
- |
Welding of low alloy
CrMo pearl tic steels, such as high temperature, high pressure
boiler pipeline, petroleum cracking equipment, working temperature of which
is below 540oC .
|
|
CHH317 |
Low hydrogen sodium
|
GB E5515-B2-V
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
<=0.90
0.70
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.80-1.50
1.10
|
0.40-0.65
0.50
|
0.10-0.35
0.20
|
- |
>=440
520
|
>=540
620
|
>=17
23
|
- |
Welding of low alloy
CrMo pearl tic steels, such as high temperature, high pressure
boiler pipeline, petroleum cracking equipment, working temperature of which
is below 540oC .
|
|
CHH327 |
Low hydrogen sodium
|
GB E5515-B2-VW
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
0.70-1.10
0.80
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.80-1.50
1.40
|
0.70-1.00
0.80
|
0.20-0.35
0.25
|
W
0.25-0.50
|
>=440
520
|
>=540
620
|
>=17
23
|
- |
Welding of low alloy
15CrMoV steels working temperature of which is below 570oC
.
|
|
CHH337 |
Low hydrogen sodium
|
GB E5515-B2-VNb
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
<=0.90
0.80
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
0.80-1.50
1.40
|
0.70-1.00
0.90
|
0.15-0.40
0.15
|
Nb
0.10-0.25
|
>=440
530
|
>=540
630
|
>=17
22
|
- |
Welding of low alloy
CrMoV steels working temperature of which is below 570oC
.
|
|
CHH347 |
Low hydrogen sodium
|
GB E5515-B3-VWB
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.07
|
<=1.00
0.80
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
1.50-2.50
2.20
|
0.30-0.80
0.50
|
0.20-0.60
0.
|
W
0.25-0.60
|
>=440
550
|
>=540
650
|
>=17
24
|
- |
Welding of
corresponding low alloy steel structures, such as high temperature,
high pressure turbo generator unit, boiler pipeline, working temperature
of which is below 620oC .
|
|
CHH347A |
Low hydrogen sodium
|
GB E5515-B3-VWB
|
F, V,
OH, H
|
DC+
|
<=0.12
-
|
0.40-0.80
-
|
0.40-0.80
-
|
<=0.035
-
|
<=0.040
-
|
1.80-2.30
-
|
0.50-0.80
-
|
0.25-0.45
-
|
Ti
0.08-0.18
|
- |
>=490
-
|
>=14
|
- |
Welding of
corresponding low alloy steel structures, such as high temperature,
high pressure turbo generator unit, boiler pipeline, working temperature
of which is below 620oC .
|
|
CHH407 |
Low hydrogen sodium
|
AWS E9015-B3
GB E6015-B3
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.08
|
<=0.90
0.75
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
2.00-2.50
2.20
|
0.90-1.20
1.00
|
- |
- |
>=490
6000
|
>=590
670
|
>=15
22
|
20oC
>=
27
|
Welding of
corresponding low alloy steel structures, such as high temperature,
high pressure turbo generator unit, boiler pipeline, working temperature
of which is below 620oC .
|
|
CHH417 |
Low hydrogen sodium
|
GB E5515-B3-VNb
|
F, V,
OH, H
|
DC+
|
0.05-0.12
0.08
|
<=1.00
0.80
|
<=0.60
0.40
|
<=0.035
0.010
|
<=0.035
0.020
|
2.40-3.00
2.60
|
0.70-1.00
0.80
|
0.25-0.50
0.
|
Nb
0.35-0.65
|
>=440
550
|
>=540
670
|
>=17
22
|
- |
Welding of low alloy
12Cr3MoVSiTiB pearl tic steel structures, such as high temperature
high pressure boiler pipeline, working temperature of which is below 620oC
.
|
|
CHH507 |
Low hydrogen sodium
|
AWS E502-15
GB E1-5MoV-15
|
F, V,
OH, H
|
DC+
|
<=0.12
-
|
0.50-0.90
-
|
<=0.50
-
|
<=0.30
-
|
<=0.35
-
|
4.50-6.00
-
|
0.40-0.70
-
|
0.10-0.35
-
|
Cu
<=0.50
|
- |
>=540
-
|
>=14
-
|
- |
Welding of
Cr-Mo pearlitic steels, working temperature is below 620oC.
|
|
CHH707 |
Low hydrogen sodium
|
-
|
F, V,
OH, H
|
DC+
|
<=0.15
|
0.50-1.00
|
<=0.50
|
<=0.30
|
<=0.35
|
8.50-10.0
|
0.70-1.00
|
- |
Cu
<=0.50
|
- |
>=590
-
|
>=16
-
|
- |
Welding of Cr9Mo
stainless steel structures for transmission of heat.
|
|
CHH807 |
Low hydrogen sodium
|
GB E1-11MoVNi-15
|
F, V,
OH, H
|
DC+
|
<=0.19
|
0.50-1.00
|
<=0.50
|
<=0.30
|
<=0.35
|
9.50-11.5
|
0.60-0.90
|
0.20-0.45
|
Ni
0.60-0.90
|
- |
>=730
-
|
>=15
-
|
- |
Welding of 1Cr11MoV
stainless steel structures, such as vanes of high pressure steam turbine,
working temperature of which is below 560oC .
|
|
|
|